Property
170 mil
180 mil
190 mil
200 mil
Test Method
Construction and Composition
Ceramic filled silicone elastomer
Ceramic filled silicone elastomer
Ceramic filled silicone elastomer
Ceramic filled silicone elastomer
 
Color
Mint
Mint
Mint
Mint
Visual
Thickness
0.170" (4.32 mm)
0.180" (4.57 mm) 0.190" (4.83mm) 0.200" (5.08 mm)  
Thickness Tolerance +/- 0.017" (+/- 0.432 mm) +/- 0.018" (+/- 0.457 mm) +/- 0.019" (+/- 0.483 mm) +/- 0.020" (+/- 0.508 mm)  
Density
1.75 g/cc
1.75 g/cc
1.76 g/cc
1.75 g/cc
He Pycnometer
Hardness
27 Shore OO
27 Shore OO
27 Shore OO
27 Shore OO
ASTM D2240
Tensile Strength
15 psi
15 psi
15 psi
15 psi
ASTM D412
Elongation %
76
76
76
76
ASTM D412
Deflection vs. Pressure Chart
Click Here
Click Here
Click Here
Click Here
Deflection %
@ 10 psi
36.36
36.87
37.335
37.8
@ 50 psi
68.69
69.48
70.24
71
@ 100 psi
82.9
83.6
84.3
85
Outgassing TML
0.56
0.56
0.56
0.56
ASTM E595
Outgassing CVCM
0.1
0.1
0.1
0.1
ASTM E595
Temperature Range
-40 to 160°C
-40 to 160°C
-40 to 160°C
-40 to 160°C
Thermal Conductivity
1.2 w/mK
1.2 w/mK
1.2 w/mK
1.2 w/mK
ASTM D5470 (modified)
Thermal Resistance
@ 10 psi 2.964°C in²/W
3.062°C in²/W
3.154°C in²/W
3.240°C in²/W
ASTM D5470 (modified)
@ 69 KPa
19.01°C-cm²/W
19.64°C-cm²/W
20.23°C-cm²/W
20.78°C-cm²/W
Thermal Impedance vs. Pressure
Click Here
Click Here
Click Here
Click Here
Compression Set (%) (24 hour hold)
17.22
ASTM D395-03 (modified)
Extractable Silicone
16%
16%
16%
16%
CTM_Belcore
Thermal Expansion (ppm/°C)
IPC-TM-650 2.4.24
38 - 58°C
517
517
517
517
58 - 103°C
754
754
754
754
103 - 135°C
906
906
906
906
Breakdown Voltage (VAC)
>10,000
>10,000
>10,000
>10,000
ASTM D149
Volume Resistivity
6.00E+12
6.00E+12
6.00E+12
6.00E+12
ASTM D257
Dielectric Constant @ 1 kHz/1 mHz
5.5/4.4
5.5/4.4
5.5/4.4
5.5/4.4
ASTM D150